Nozzle School · Troubleshooting
Under-Extrusion: Causes and Fixes for Gaps and Thin Layers
Why your 3D printer under-extrudes, with gaps, thin walls and weak layers, and how to fix it: clogs, temperature, speed, extruder grip and flow.
Under-extrusion is when your printer pushes out less plastic than the slicer asked for, so you get gaps between lines, thin or see-through walls and weak, crumbly layers. You fix it by finding what is starving the nozzle, usually a partial clog, a nozzle that is too cold for the speed, or an extruder that is slipping, and only then fine-tuning the flow setting.
This guide shows how to recognise under-extrusion, how to tell it apart from faults that look similar, and walks through every common cause with the settings to change in OrcaSlicer, Bambu Studio, PrusaSlicer and Cura. It works for any FDM printer, direct drive or Bowden.
Quick fix checklist
Work down this list in order and re-print a small test (a 20 mm cube or a single-wall box) after each change:
- Check the filament diameter in the slicer matches your spool (almost always 1.75 mm).
- Push filament through by hand on a hot nozzle. A weak, curling thread means a partial clog.
- Raise the nozzle temperature by 5–10 °C, staying inside the filament’s range.
- Slow down, or set a maximum volumetric speed so fast infill can’t outrun the hotend.
- Check the extruder: tension, a clean drive gear and no ground-down filament.
- Make sure the spool turns freely and the filament path has no kinks or tangles.
- Check the hotend fan is spinning, to rule out heat creep.
- Dry the filament if it pops, hisses or prints rough.
- Calibrate flow (and the extruder’s steps) last, once everything above is right.
Test prints on the way from failure to a clean part.Photo: Dbsnp ·CC BY-SA 4.0 ·Wikimedia Commons
Another failed Benchy: messy, sagging layers.Photo: 3DBenchy ·CC BY 2.0 ·Wikimedia Commons
The calibration cube a few layers in.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
Molten plastic leaving the nozzle.Photo: David Elliott from UK ·CC BY 2.0 ·Wikimedia Commons
A first layer close up: lines pressed together on the bed.Photo: hdaniel ·CC BY-SA 2.0 ·Wikimedia Commons
Solid filament above the heat break, molten filament in the heater block.
What is under-extrusion?
Under-extrusion means the nozzle lays down thinner lines than planned. The slicer works out exactly how much filament each line needs; if less arrives, the lines don’t touch their neighbours and the part ends up with holes.
How to recognise it:
- Gaps between lines on the top surface, so you can see the infill underneath.
- Thin walls with holes, or walls you can see light through.
- Missing or broken layers, especially part way up a tall print.
- Weak, spongy infill that crushes easily, with strands that don’t join up.
- Rough, uneven or “dry” looking surfaces instead of smooth, glossy lines.
- Parts that are slightly undersized or snap along the layer lines.
It can be constant (the whole print is thin, which points at a setting such as filament diameter or flow) or intermittent (fine in some places, starved in others, which points at a clog, speed, a slipping extruder or a snag in the filament path). Noticing which one you have narrows the search a lot.
Gyroid infill printed: strong in every direction.Photo: A7N8X ·CC BY-SA 4.0 ·Wikimedia Commons
Inside a print: 40% grid infill.Photo: Sumanbargavr ·CC BY-SA 4.0 ·Wikimedia Commons
Benchy cut open: walls, infill and overhangs in one small boat.Photo: CreativeTools: https://www.thingiverse.com/Cr… ·CC0 ·Wikimedia Commons
A twisted vase printed in a single wall.Photo: Sumanbargavr ·CC BY-SA 4.0 ·Wikimedia Commons
A 20 mm calibration cube, often the first print.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
Printed Benchys in different filaments.Photo: 3DBenchy ·CC BY 2.0 ·Wikimedia Commons
Faults that look like under-extrusion but aren’t
- Nozzle too high on the first layer: round lines that don’t touch, only on layer one. That’s Z offset, not flow.
- Gaps only above infill on the top layers (“pillowing”): too few top layers or too sparse infill to bridge over. Add top layers instead of more flow.
- Layer shifts: whole layers jump sideways. That’s a mechanical or belt problem, not extrusion.
- Over-extrusion: blobs, rough sides and an elephant’s foot. The opposite fault, sometimes caused by over-correcting under-extrusion.
- A clicking extruder: this is a symptom that often comes with under-extrusion. See why the extruder clicks.
Too high: round lines that don't touch or stick.
Cross-section, too high: the line stays round.
Z offset +0.06 mm: gap 0.26 mm · line 0.37 × 0.26 mm · too high · gaps between lines.
Nozzle height decides the first layer: too close, just right, too far.Photo: Stemfie3D ·CC BY-SA 4.0 ·Wikimedia Commons
Layer shifting: the layers jump sideways part way up the print.Photo: A7N8X ·CC BY-SA 4.0 ·Wikimedia Commons
A print that broke loose partway through.Photo: EwkaC ·CC BY-SA 4.0 ·Wikimedia Commons
The same failure from the side: layers stop where the part moved.Photo: EwkaC ·CC BY-SA 4.0 ·Wikimedia Commons
Too low, the pressure rises until the extruder skips.
How plastic gets from the spool to the part
To fix under-extrusion it helps to know the path the filament takes, because a problem anywhere along it starves the nozzle:
- The spool has to turn freely so the filament can be pulled off it.
- The extruder grips the filament between drive gears and pushes it forward, a precise number of millimetres per command.
- On a Bowden printer it travels down a PTFE tube; on a direct drive printer the extruder sits right on top of the hotend.
- The hotend melts it: cold at the top (heatsink and heat break), hot at the bottom (heater block).
- The molten plastic is squeezed out through a 0.4 mm nozzle (on most printers) and laid as a flattened line.
The extruder only pushes; it has no idea whether plastic actually came out. If the gears slip, the hotend can’t melt fast enough, or the nozzle is partly blocked, the printer carries on as if nothing were wrong and you get thin lines.
nozzle 210 °C · heatsink 38 °C · feed 2.0 mm/s · melting in block
- drag ↕ feed rate
- ↑ ↓ feed ±0.5 mm/s
- Space stop / start feed
- F hotend fan on / off
- Home reset
A V6-style hotend, cut away so you can see the filament inside.
The print head: extruder on top, finned heatsink, heater block and nozzle.
A 1 kg spool of 1.75 mm filament on a roller stand.
The finned heatsink keeps the top of the hotend cold.
The heater block holds the heater cartridge and the thermistor.
A brass 0.4 mm nozzle laying a thin strand.
asked 4.9 mm³/s · got 4.9 mm³/s · line 0.45 mm · lines touch
- ↑ ↓ print speed ±10 mm/s (20–250); or drag ↕
- ← → nozzle temperature ±5 °C (180–240)
- − + flow ratio ±2 % (80–110)
- T extruder tension: loose, normal, tight
- C partial clog: none, 30, 50, 80 %
- Home reset
Cause and fix reference
| What you see | Most likely cause | Fix | Step |
|---|---|---|---|
| Whole print thin, even slow walls | Wrong filament diameter or flow setting | Check diameter, then calibrate flow | 1, 9 |
| Thin, uneven lines even at low speed; weak thread when pushed by hand | Partial clog or worn nozzle | Push through hot, cold pull, new nozzle | 2 |
| Weak layers that snap easily, dull surface | Nozzle too cold | Raise temperature 5–10 °C | 3 |
| Walls fine, fast infill and solid areas starved | Printing faster than the hotend can melt | Slow down, set max volumetric speed | 4 |
| Clicking, filament with chewed notches | Extruder slipping | Tension, clean or replace the gear | 5 |
| Under-extrusion in bursts, worse late in the spool | Drag in the filament path, tangle | Free the spool, fix kinks and the PTFE tube | 6 |
| Good at the start, starved after 10–30 minutes | Heat creep | Check the hotend fan, reduce retraction | 7 |
| Popping, hissing, bubbly or rough lines | Wet filament | Dry the spool | 8 |
| Gaps at the start of lines after travel | Retraction or prime settings | Reduce retraction, check restart settings | 10 |
Step 1: Check the filament diameter setting
Try this first, because it takes ten seconds. The slicer calculates extrusion from the filament diameter you give it. Almost every printer now uses 1.75 mm filament; some older or professional printers use 2.85 mm (often sold as “3 mm”).
- If your profile says 2.85 mm but you print 1.75 mm filament, the printer feeds far too little plastic. If it says 1.75 mm on a 2.85 mm printer, it badly over-extrudes.
- Good filament holds its diameter to within a few hundredths of a millimetre. Cheap filament that runs thin starves the nozzle in patches.11Plastic delivered goes with the square of the diameter: filament that is really 1.70 mm instead of 1.75 mm carries about 6% less plastic per millimetre fed.
- If you suspect the spool, measure it with calipers in several places along a metre or so. Readings that wander a lot mean the spool, not the printer, is the problem.
Read the label: material, 1.75 mm diameter, 1 kg.Photo: John Abella from Outside Philadelphia, USA ·CC BY 2.0 ·Wikimedia Commons
A spool of white filament.Photo: Creative Tools ·CC BY 2.0 ·Wikimedia Commons
PLA: the beginner's filament.Photo: Richardspa ·CC0 ·Wikimedia Commons
Refill filament: a coil and a reusable spool.Photo: Suit ·CC BY-SA 4.0 ·Wikimedia Commons
Step 2: Clear a partial clog or replace the nozzle
A partly blocked nozzle is the most common cause of intermittent under-extrusion. Some plastic gets through, so the print carries on, but lines come out thin and uneven, and often the extruder clicks.
How to recognise it:
- Lines stay thin even at slow speed and normal temperature.
- When you push filament through a hot nozzle by hand, it comes out weak, thin or curling sideways instead of a steady, straight thread.
- It started after a material change (for example PETG back to PLA) or after the printer sat hot and idle.
The fix, gentlest first:
- Heat to printing temperature and push filament through for a few centimetres.
- Raise the temperature 10–20 °C and push again to soften stubborn leftovers.
- Do a cold pull to drag debris out with the filament.
- Replace the nozzle. Brass nozzles wear, especially after abrasive filaments (glow-in-the-dark, carbon fibre, wood-fill), and a worn or damaged one never flows quite right again.
Full instructions for each method are in how to unclog a 3D printer nozzle.
A heater block in a silicone sock, with the nozzle below and heat break above.Photo: A7N8X ·CC0 ·Wikimedia Commons
The nozzle threads into the heater block.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
The mount that holds the hotend to the carriage.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
The "blob of death": plastic that leaked and wrapped the hotend.Photo: LunaEatsTuna ·CC BY-SA 4.0 ·Wikimedia Commons
A thin strand pulled from the nozzle: where strings begin.Photo: David Elliott from UK ·CC BY 2.0 ·Wikimedia Commons
Ooze: a drop of molten plastic forming at the nozzle.Photo: David Elliott from UK ·CC BY 2.0 ·Wikimedia Commons
Step 3: Raise the nozzle temperature
Colder plastic is thicker and harder to push through the nozzle. Too cold, and the extruder can’t force enough of it out in time, so the lines thin out and the layers don’t fuse properly. The print may look dull and break cleanly along the layer lines.
- Raise the nozzle temperature in 5 °C steps and re-test.
- Stay inside the filament maker’s range. Going far above it causes stringing, blobs and burnt plastic.
- Print faster, print hotter: if you speed up, you usually need the upper half of the range so the plastic melts in time.
| Filament | Typical nozzle range | Start at |
|---|---|---|
| PLA | 190–220 °C | 205 °C |
| PETG | 220–250 °C | 235 °C |
| TPU | 210–235 °C | 220 °C |
| ABS / ASA | 230–260 °C | 245 °C |
A temperature tower (built into OrcaSlicer, Bambu Studio and PrusaSlicer, or downloadable for Cura) shows you the whole range on one print. Pick a section with strong layers and a clean surface. For more on what each material needs, see PLA vs PETG.
190 °C, 0.8 mm retraction: no strings.
200 °C, 0.8 mm retraction: few strings.
210 °C, 0.8 mm retraction: few strings.
220 °C, 0.8 mm retraction: some strings.
Flexible filament: label shows its print temperature.Photo: Sweetclara ·CC BY-SA 4.0 ·Wikimedia Commons
A spool of ABS.Photo: Tatár Lehel ·CC BY-SA 3.0 ·Wikimedia Commons
A 1 kg spool of PETG, sealed with desiccant.Photo: Suit ·CC BY-SA 4.0 ·Wikimedia Commons
The control box shows nozzle and bed temperature, height and progress.
Step 4: Slow down to what the hotend can melt
A hotend can only melt so much plastic per second. Ask for more and the plastic leaves the nozzle half-melted, the pressure climbs and the line comes out thin. The classic sign: walls print fine but fast infill and large solid areas are starved, because those are printed fastest and widest.
The limit is called maximum volumetric flow, in mm³/s. Roughly:
flow (mm³/s) ≈ line width × layer height × print speed
So a 0.45 mm line at 0.2 mm layers and 100 mm/s asks for about 9 mm³/s. Thicker layers or wider lines raise it quickly: the same speed at 0.3 mm layers asks for about 13.5 mm³/s.
| Hotend type | Typical max flow for PLA |
|---|---|
| Standard V6-style hotend | roughly 10–15 mm³/s |
| High-flow hotends (longer melt zone or core heating) | roughly 20–35 mm³/s or more |
These are typical figures; the real limit depends on your hotend, the filament and the temperature, so check your printer maker’s recommendation. OrcaSlicer and Bambu Studio also have a max flow calibration test.
What to do:
- Lower print speed, especially infill speed, by 20–30% and re-test.
- Set maximum volumetric speed in the slicer a little below your hotend’s limit. The slicer then slows down automatically wherever a feature would ask for too much.
- If you want speed, raise temperature a little or use a high-flow hotend, rather than just pushing faster.
Feed 1 mm/s: nozzle 210 °C · heatsink 38 °C · feed 1.0 mm/s · melting in block.
Feed 2 mm/s: nozzle 210 °C · heatsink 38 °C · feed 2.0 mm/s · melting in block.
Feed 3 mm/s: nozzle 210 °C · heatsink 38 °C · feed 3.0 mm/s · melting in block.
Feed 4 mm/s: nozzle 210 °C · heatsink 38 °C · feed 4.0 mm/s · melting in block.
Feed 6 mm/s: nozzle 210 °C · heatsink 38 °C · feed 6.0 mm/s · melting in block.
Feed 8 mm/s: nozzle 210 °C · heatsink 38 °C · feed 8.0 mm/s · too fast.
An enclosed CoreXY printer on a home desk.Photo: Mortymore ·CC BY 2.0 ·Wikimedia Commons
A CoreXY print head on a QIDI printer.Photo: Haroldbarlow8911 ·CC BY-SA 4.0 ·Wikimedia Commons
A modern toolhead: extruder, hotend and fans in one housing.Photo: disinterpreter ·CC BY-SA 2.0 ·Wikimedia Commons
Where to find these settings in your slicer
| Setting | OrcaSlicer / Bambu Studio | PrusaSlicer | Cura |
|---|---|---|---|
| Filament diameter | Filament settings → Diameter | Filament Settings → Filament → Diameter | Material profile (Preferences → Materials) |
| Flow ratio | Filament settings → Flow ratio | Filament Settings → Filament → Extrusion multiplier | Material → Flow |
| Nozzle temperature | Filament settings → Nozzle temperature | Filament Settings → Filament → Temperature → Nozzle | Material → Printing Temperature |
| Max volumetric speed | Filament settings → Volumetric speed limitation | Filament Settings → Advanced → Max volumetric speed | no direct setting; lower Print Speed instead |
| Print / infill speed | Process → Speed | Print Settings → Speed | Speed → Print Speed / Infill Speed |
| Nozzle diameter | Printer settings → Extruder → Nozzle diameter | Printer Settings → Extruder 1 → Nozzle diameter | Machine Settings → Extruder 1 → Nozzle size |
| Retraction length | Printer settings → Extruder → Retraction | Printer Settings → Extruder 1 → Retraction → Length | Travel → Retraction Distance |
Menu names move between slicer versions. If you can’t find a setting, type its name into the slicer’s settings search box.
Step 5: Check the extruder grip
The extruder presses the filament against a toothed drive gear with a spring and a tension screw or arm. If it can’t grip, the gear spins but the filament doesn’t move as far as it should.
How to recognise it:
- The extruder clicks or the gear makes a grinding noise.
- Filament you pull out has chewed notches or a flattened, shiny patch where the gear spun on it.
- White or coloured plastic dust around the gear.
The fix:
- Set the tension so the filament is gripped firmly but not crushed. Too loose slips; too tight flattens the filament (especially TPU) and can jam it.
- Clean the drive gear with a small brush or pick. Packed plastic dust stops the teeth biting.
- Replace worn gears with rounded teeth. They’re cheap and wear out on every printer eventually.
- If the filament was ground down, cut above the damaged section and reload.
clamp 19 N · grips · fed 0.0 of 0 mm · mark at 120.0 mm
- drag ↕ tension (thumb nut)
- ↑ ↓ tension ±1 turn, 0–6
- Space feed 100 mm (E-steps test); again to re-mark
- R retract 5 mm
- − + firmware E-steps ±1 (80–110)
- Home reset
An extruder motor with its tension knob.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
An assembled extruder before it goes on the printer.Photo: John Abella ·CC BY 2.0 ·Wikimedia Commons
A geared extruder on a Prusa i3.Photo: John Abella from Outside Philadelphia, USA ·CC BY 2.0 ·Wikimedia Commons
An early Ultimaker extruder: a big gear pushing filament.Photo: jabella ·CC BY 2.0 ·Wikimedia Commons
The extruder knob turns back by the retraction distance.
A small fan cooling the extruder assembly.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
A dual-nozzle head: two hotends side by side.Photo: Creative Tools from Halmstad, Sweden ·CC BY 2.0 ·Wikimedia Commons
The toolhead rides the gantry; cable chains carry its wires.Photo: disinterpreter ·CC BY-SA 2.0 ·Wikimedia Commons
Step 6: Check the spool and filament path
If the spool or filament path resists, the extruder spends its force pulling instead of pushing, and the nozzle gets less plastic. This usually shows as under-extrusion that comes and goes, or gets worse near the end of a spool where the filament is coiled more tightly.
- Make sure the spool turns freely on its holder. A stiff holder can be enough to cause slipping.
- Look for a crossed or tangled loop where one strand is trapped under another. It can lock the spool solid.
- Check the PTFE tube and guides for kinks or sharp bends.
- On Bowden printers, check the tube is pushed fully into the hotend and the collet holds it. A gap at the bottom lets plastic pool and cause jams and uneven flow.22When a Bowden tube backs out of its fitting, molten plastic fills the gap and hardens into a ring. That restriction looks exactly like a partial clog, and pushing the tube back in after cleaning it out fixes it.
Crossed filament: a loop that can tangle and stop the extruder.Photo: SuperBlobMonster ·CC BY-SA 3.0 ·Wikimedia Commons
A simple spool holder lets the spool turn freely.Photo: Creative Tools ·CC BY 2.0 ·Wikimedia Commons
Open the reusable spool…Photo: Suit ·CC BY-SA 4.0 ·Wikimedia Commons
…drop the coil in…Photo: Suit ·CC BY-SA 4.0 ·Wikimedia Commons
…and close it. Cut the ties last.Photo: Suit ·CC BY-SA 4.0 ·Wikimedia Commons
The Bowden tube enters through a push-fit collet.
The gantry and print head of a bed-slinger.Photo: kenming Wang ·CC BY-SA 2.0 ·Wikimedia Commons
The X gantry: the print head rides along it on a belt.
Step 7: Rule out heat creep
Heat creep is when heat travels up past the heat break and softens the filament too early. Soft filament swells and drags on the walls of the cold zone, so less and less gets through.
How to recognise it: the print starts well, then under-extrudes or stops after 10–30 minutes, often with clicking. It’s more common with PLA in warm rooms or enclosures.
- Check the hotend fan (the one on the heatsink, not the part-cooling fan). It must spin whenever the hotend is hot. Clean dust off it and the heatsink fins.
- Reduce retraction. Long retractions pull molten plastic up into the cold zone.
- Keep PLA cool: open the door or lid of an enclosed printer.
Fan off: heat creeps up the heatsink and the filament softens too high.
The hotend fan cools the heatsink. It must run whenever the hotend is hot.
Heater and thermistor wires run to the terminal block.
Too much retraction pulls melt up into the heat break.
Retraction 2.4 mm at 205 °C: no strings, but melt is pulled into the heat break.
Inside the hotend: solid filament above, melt below.
Step 8: Dry the filament
Wet filament boils in the hotend. The steam makes bubbles and voids in the line, so less solid plastic lands where it should, and the surface turns rough or fuzzy. You’ll often hear popping or crackling while it prints.
- Dry it in a filament dryer or food dehydrator for 4–6 hours.
- Typical temperatures: PLA 45–50 °C, PETG 60–65 °C, TPU 50–55 °C. Check the filament maker’s guidance.
- Store dried spools sealed with fresh desiccant.
An open spool of PLA left out in the air.Photo: SuperBlobMonster ·CC BY-SA 3.0 ·Wikimedia Commons
Filament comes in almost every colour.Photo: westonhighschool library ·CC BY-SA 2.0 ·Wikimedia Commons
An enclosure keeps heat in for ABS and ASA.Photo: -stk ·CC BY-SA 4.0 ·Wikimedia Commons
Step 9: Calibrate flow and extruder steps
Only do this once the hardware causes above are ruled out. Turning up flow to hide a clog or a slipping extruder just moves the problem around.
Check the extruder pushes the right length
The printer’s firmware has a setting for how far the extruder motor turns per millimetre of filament: E-steps on Marlin printers, rotation_distance on Klipper. Most printers ship correct, but it’s worth checking after changing the extruder.
- Heat the nozzle to printing temperature.
- Mark the filament 120 mm above the extruder entry.
- Extrude 100 mm slowly (about 1–2 mm/s, so the hotend isn’t the limit).
- Measure from the entry to the mark. It should be 20 mm. If it isn’t, the extruder pushed more or less than 100 mm.
- New E-steps = old E-steps × 100 ÷ actual length extruded. On Marlin,
M503shows the current value,M92 E<value>sets it andM500saves it. Klipper uses the same idea with rotation_distance (old × actual ÷ 100) in printer.cfg.
Fine-tune the flow ratio
Flow ratio (Extrusion multiplier in PrusaSlicer, Flow in Cura) scales every line up or down. It accounts for small differences between filaments.
- Most filaments land between 0.92 and 1.05. Change it in 2–5% steps.
- OrcaSlicer and Bambu Studio have a built-in flow rate calibration that prints patches at different flow values; pick the smoothest top surface.
- Or print a single-wall cube in vase mode, measure the wall with calipers and set: new flow = old flow × line width ÷ measured wall.
- Set flow per filament, not for the printer, because each spool and material differs.
A printed bowl: walls only, no infill.Photo: Sumanbargavr ·CC BY-SA 4.0 ·Wikimedia Commons
A screw-top box: threads print well at 0.2 mm layers.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
The mainboard: the printer's brain.Photo: kenming Wang ·CC BY-SA 2.0 ·Wikimedia Commons
Stepper drivers on the mainboard, one per motor.Photo: kenming Wang ·CC BY-SA 2.0 ·Wikimedia Commons
Step 10: Gaps after travel moves
If lines start thin or with a gap right after a travel move, and the rest of the line is fine, look at retraction:
- Too much retraction pulls the filament back further than it gets pushed forward again, or pulls melt into the cold zone where it sticks. Try the low end: 0.5–1 mm direct drive, 4–6 mm Bowden.
- Extra length on restart (Retraction Extra Prime Amount in Cura) adds a little plastic after each retraction. Leave it at 0 unless you see consistent gaps at line starts, then try small amounts.
- Wipe and coasting remove plastic at the end of lines. Too much coasting leaves gaps; turn it down or off.
- Pressure advance (Linear Advance on Marlin) set too high can thin out line starts and corners. Re-run its calibration if you changed it.
To learn how retraction works and how to tune it without causing these gaps, see what is retraction and the stringing guide.
Retraction 0.0 mm at 205 °C: many strings.
Retraction 0.8 mm at 205 °C: few strings.
Retraction 1.6 mm at 205 °C: no strings.
Retraction 2.8 mm at 205 °C: no strings, but melt is pulled into the heat break.
A stringing test: two thin towers and a head that travels between them.
The dial reads retraction in 0.25 mm steps.
A print head at work over a plate of small parts.Photo: Neon Tommy ·CC BY-SA 2.0 ·Wikimedia Commons
Stringing on a two-colour Benchy, where travel moves cross open air.Photo: 3DBenchy ·CC BY 2.0 ·Wikimedia Commons
Under-extrusion on the first layer only
A thin, gappy first layer with a fine rest of the print is almost never a flow problem:
- Nozzle too high: round lines with gaps between them. Lower the Z offset in small steps.
- Nozzle too low: the nozzle presses against the bed, plastic can’t get out, the extruder clicks and the line is scraped thin and see-through.
- Uneven bed: good in one corner, gappy in another. Level the bed or re-run the mesh.
See what is Z offset, how to level a 3D printer bed and first layer not sticking.
gap 0.20 mm · line 0.45 × 0.20 mm · good squish
- Drag ↕ raise / lower the nozzle
- ↑ ↓ one babystep, 0.02 mm (Shift: 0.10)
- 1 2 3 too high · good · too low
- Home back to 0.00
Z offset right: slightly squished lines that touch.
Too low: lines squashed thin, and the extruder struggles.
Cross-section, too low: the line is pressed into a sheet.
A probed 5 × 5 mesh across the bed.
Turn a knob and the old mesh no longer matches the bed. Probe again.
The first layers going down on a heated bed.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
Settings by material
| Material | Under-extrusion risk | Nozzle | Watch out for |
|---|---|---|---|
| PLA | Low | 190–220 °C | Heat creep in warm enclosures; speed above the hotend’s limit |
| PETG | Medium | 220–250 °C | Printing too cold; moisture |
| TPU | High | 210–235 °C | Soft filament buckles in the extruder; print slowly with gentle tension |
| ABS / ASA | Medium | 230–260 °C | Too cold for the speed |
| Filled (wood, carbon fibre, glow) | High | per label | Wears brass nozzles; use a hardened nozzle, often 0.6 mm |
Start from the maker’s profile for the exact filament before changing anything.
A table of small prints.Photo: Trevor Prentice ·CC BY-SA 2.0 ·Wikimedia Commons
A two-colour Benchy.Photo: 3DBenchy ·CC BY 2.0 ·Wikimedia Commons
A working wrench printed in one piece.Photo: Creative Tools from Halmdstad, Sweden ·CC BY 2.0 ·Wikimedia Commons
When under-extrusion won’t go away
If you’ve worked through every step:
- Try a fresh spool from another brand to rule out a bad batch.
- Reset to the stock profile and change one thing at a time.
- Replace the nozzle even if it looks fine. Wear inside isn’t visible.
- Check the heater and thermistor. If the reading is wrong, the nozzle may be colder than the screen says. A loose thermistor or a weak heater cartridge can cause this.
- Check the extruder motor and its wiring. A loose connector can make it skip steps.
Your action plan
- Confirm 1.75 mm (or 2.85 mm) filament diameter in the slicer.
- Push filament through hot; clear any clog or swap the nozzle.
- Raise the temperature 5–10 °C.
- Slow down or set a max volumetric speed.
- Fix extruder tension and clean the gear.
- Free the spool and the filament path.
- Check the hotend fan.
- Dry the filament.
- Calibrate E-steps, then flow ratio.
FAQ
What does under-extrusion look like?
Gaps between lines on top surfaces, thin or see-through walls, missing layers and weak, stringy infill that doesn’t join up. The surface often looks dry and rough instead of smooth and glossy.
Should I just increase the flow rate?
Only once you’ve ruled out clogs, temperature, speed and extruder grip. Flow ratio is for small corrections of a few percent. Turning it up to hide a hardware problem leads to over-extrusion in some places and still-starved lines in others.
Why does my printer under-extrude only on infill?
Infill is usually printed faster and wider than walls, so it asks for more plastic per second. If it’s starved while walls look fine, you’re over the hotend’s maximum volumetric flow. Lower infill speed or set a max volumetric speed.
Can a worn nozzle cause under-extrusion?
Yes. Nozzles wear inside, especially brass ones after abrasive filaments, and debris builds up over time. A new nozzle is cheap and often fixes under-extrusion that nothing else will.
Why did my prints start under-extruding suddenly?
Usually a partial clog, a new spool that’s wet or a different diameter, a tangle on the spool, or a hotend fan that has stopped. Check those before changing settings.
Is under-extrusion the same as a clogged nozzle?
No. A clog is one cause of under-extrusion. Others include a cold nozzle, printing too fast, a slipping extruder and wrong slicer settings.
Does under-extrusion make parts weaker?
Yes. Gaps between lines and poorly fused layers mean less plastic holding the part together, so under-extruded parts crack and snap along the layer lines much more easily.
Related guides
This guide is part of our print quality series; start with the stringing guide, the cluster’s main post. If your extruder clicks along with the gaps, read why the extruder clicks; for clogs, how to unclog a nozzle. To understand the extruder, hotend and nozzle, see parts of a 3D printer explained, and if you’re new, start with the complete beginner’s guide.