Nozzle School · Troubleshooting
Over-Extrusion: Causes and Fixes for Blobby, Oversized Prints
Why your 3D printer over-extrudes, with blobs, rough walls and oversized parts, and how to fix it: flow ratio, filament diameter, temperature and E-steps.
Over-extrusion is when your printer pushes out more plastic than the slicer planned, so lines come out too wide and the extra plastic piles up as blobs, lumpy walls, ridged top surfaces and parts that are slightly too big. You fix it by checking the settings that decide how much plastic is fed (flow ratio, filament diameter, nozzle and line width) and the extruder’s calibration, then fine-tuning flow with a short test print.
This guide shows how to recognise over-extrusion, how to tell it apart from faults that look similar, and walks through every common cause with the settings to change in OrcaSlicer, Bambu Studio, PrusaSlicer and Cura. It works for any FDM printer, direct drive or Bowden.
Quick fix checklist
Work down this list in order and re-print a small test (a 20 mm cube is enough) after each change:
- Undo recent flow changes. If you raised flow to fix gaps earlier, go back to the filament’s stock value.
- Check the filament diameter in the slicer matches your spool (almost always 1.75 mm).
- Check the nozzle size in the printer profile matches the nozzle actually fitted.
- Lower the flow ratio in 2–5% steps, or run your slicer’s flow calibration.
- Lower the nozzle temperature by 5–10 °C if you’re near the top of the filament’s range.
- Check the first layer isn’t squashed too hard (Z offset too low).
- Check the extruder’s steps (E-steps or rotation distance) if you changed the extruder or firmware.
- Tune pressure advance if the extra plastic only shows at corners and line ends.
The calibration cube a few layers in.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
A 20 mm calibration cube, often the first print.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
Molten plastic leaving the nozzle.Photo: David Elliott from UK ·CC BY 2.0 ·Wikimedia Commons
Read the label: material, 1.75 mm diameter, 1 kg.Photo: John Abella from Outside Philadelphia, USA ·CC BY 2.0 ·Wikimedia Commons
Too low: lines squashed thin, and the extruder struggles.
A brass 0.4 mm nozzle laying a thin strand.
What is over-extrusion?
Every time the printer lays a line, the slicer has already worked out how much filament that line needs, from the line width, the layer height and the length of the move. Over-extrusion means more plastic arrives than that. The extra has to go somewhere, so the line spreads wider, bulges up, or gets pushed sideways into its neighbours.
How to recognise it:
- Rough, lumpy or wavy walls instead of smooth, even layer lines.
- Blobs and zits on the surface, especially at the start and end of lines.
- Ridged or “plowed” top surfaces, where the nozzle drags through extra plastic and leaves raised edges between lines.
- Parts that come out oversized: a 20 mm cube measures a bit over 20 mm on X and Y, and holes come out too small.
- Parts that don’t fit together, such as screw-top lids that bind or pegs that won’t go in.
- The nozzle scraping or knocking on the top layers, sometimes with a ticking sound or a print that gets knocked loose.
- Stringy hairs and sharp, crusty edges, because plastic keeps oozing when the nozzle moves.
Like under-extrusion, it can be constant (every layer is too fat, which points at a setting such as flow, filament diameter or E-steps) or local (only the first layer, only corners, only the top surface). Knowing which one you have tells you where to look first.
A screw-top box: threads print well at 0.2 mm layers.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
A working wrench printed in one piece.Photo: Creative Tools from Halmdstad, Sweden ·CC BY 2.0 ·Wikimedia Commons
A printed maze puzzle.Photo: Sumanbargavr ·CC BY-SA 4.0 ·Wikimedia Commons
Printed Benchys in different filaments.Photo: 3DBenchy ·CC BY 2.0 ·Wikimedia Commons
A table of small prints.Photo: Trevor Prentice ·CC BY-SA 2.0 ·Wikimedia Commons
Gyroid infill printed: strong in every direction.Photo: A7N8X ·CC BY-SA 4.0 ·Wikimedia Commons
Faults that look like over-extrusion but aren’t
- Elephant’s foot: only the bottom few layers bulge outwards. That’s the first layer being squashed or the bed being too hot, not general flow. See elephant’s foot.
- Stringing: thin hairs between separate parts of the print. Usually temperature and retraction, not flow. See how to fix stringing.
- Wet filament: popping, fuzzy, rough surfaces that look like too much plastic, but are steam bubbles. See how to dry filament.
- Ringing or ghosting: ripples on walls just after corners. That’s vibration from the motion system, not extra plastic.
- Under-extrusion after an over-correction: if you lowered flow too far, you’ll see gaps instead. The opposite fault is covered in under-extrusion.
Too low: lines squashed thin, and the extruder struggles.
Cross-section, too low: the line is pressed into a sheet.
Stringing on a two-colour Benchy, where travel moves cross open air.Photo: 3DBenchy ·CC BY 2.0 ·Wikimedia Commons
Strings and blobs across a full plate of parts.Photo: Quinn Daedal ·CC BY-SA 4.0 ·Wikimedia Commons
Hotter plastic is runnier: thinner, saggier strings.
The hull is a curved overhang test.Photo: CreativeTools: https://www.thingiverse.com/Cr… ·CC0 ·Wikimedia Commons
An open spool of PLA left out in the air.Photo: SuperBlobMonster ·CC BY-SA 3.0 ·Wikimedia Commons
A print that broke loose partway through.Photo: EwkaC ·CC BY-SA 4.0 ·Wikimedia Commons
How the printer decides how much plastic to push
Over-extrusion is almost always a numbers problem, so it helps to see which numbers the printer uses.
- The slicer works out the volume of each line: line width × layer height × length.
- It converts that volume into a length of filament, using the filament diameter you set. Thicker filament means less length is needed for the same volume.
- It multiplies by the flow ratio (Extrusion multiplier in PrusaSlicer, Flow in Cura), a correction for each filament.
- The firmware turns that length into motor steps using the extruder’s E-steps (Marlin) or rotation distance (Klipper).
- The extruder pushes that much filament into the hotend, which melts it and squeezes it out of the nozzle.
If any number in that chain is too big, every line gets too much plastic. If the numbers are right but the plastic is very runny (too hot) or pressure builds up in the nozzle and releases late, you get extra plastic in some places only.
nozzle 210 °C · heatsink 38 °C · feed 2.0 mm/s · melting in block
- drag ↕ feed rate
- ↑ ↓ feed ±0.5 mm/s
- Space stop / start feed
- F hotend fan on / off
- Home reset
flow 1.00 · 1.75 mm filament · asks 0.45 · lays 0.45 mm · flat, touching
- Drag ↔ flow ratio
- ← → flow ±0.01 (Shift ±0.05), 0.85–1.15
- ↑ ↓ filament diameter ±0.01 mm, 1.70–1.80
- 1 2 3 too low · right · too high
- Home reset: 1.00 on 1.75 mm
A V6-style hotend, cut away so you can see the filament inside.
Solid filament above the heat break, molten filament in the heater block.
The print head: extruder on top, finned heatsink, heater block and nozzle.
A 1 kg spool of 1.75 mm filament on a roller stand.
The heater block holds the heater cartridge and the thermistor.
A brass 0.4 mm nozzle laying a thin strand.
Cause and fix reference
| What you see | Most likely cause | Fix | Step |
|---|---|---|---|
| Started after you raised flow to fix gaps | Over-correction | Return flow to stock, find the real cause | 1 |
| Whole print badly oversized and lumpy | Wrong filament diameter in the slicer | Set 1.75 mm (or 2.85 mm) to match the spool | 2 |
| Very wide lines, after a nozzle swap | Nozzle size or line width mismatch | Match the profile to the fitted nozzle | 3 |
| Slightly rough walls, ridged top surface, a bit oversized | Flow ratio a little high | Calibrate flow ratio | 4 |
| Blobs, ooze, glossy droopy edges, stringing | Nozzle too hot | Lower temperature 5–10 °C | 5 |
| Only the bottom layers bulge or are see-through-flat | First layer squashed too hard | Raise the Z offset | 6 |
| Every filament over-extrudes the same amount | Extruder steps wrong | Calibrate E-steps / rotation distance | 7 |
| Bulging corners, blobs at line ends | Pressure advance off or too low | Tune pressure advance | 8 |
| Only the top surface is ridged | Too much plastic in solid layers | Lower top-surface flow, try ironing | 9 |
| Holes too small, but walls look fine | Normal plastic shrink and spread | Use hole or XY compensation | 10 |
Step 1: Undo recent flow changes
Start here if the problem appeared after you changed something. A very common route to over-extrusion is fixing gaps by turning flow up. That hides the gaps, but if the real cause was a partial clog or a cold nozzle, the next spool, or the cleaned nozzle, now gets far too much plastic.
- Set the flow ratio back to the filament profile’s default (usually 1.0, or the value the maker’s profile ships with).
- Check you didn’t raise per-feature flow (Cura has separate Wall Flow, Infill Flow and Top/Bottom Flow under Material).
- Check the printer’s own screen. Many printers have a flow or “extrusion” percentage you can change during a print, and some keep it until you reset it.
If the over-extrusion disappears and gaps come back, the real problem is under-extrusion. Fix that first, using the under-extrusion guide, and leave flow near its default.
The control box shows nozzle and bed temperature, height and progress.
An assembled Ender 3: a classic bed-slinger.Photo: kenming Wang ·CC BY-SA 2.0 ·Wikimedia Commons
A Prusa i3, the design behind many beginner printers.Photo: John Abella ·CC BY 2.0 ·Wikimedia Commons
Step 2: Check the filament diameter
The slicer turns the volume of each line into a length of filament using the diameter you give it. If it’s wrong, every line is wrong by the same amount.
- Almost every printer now uses 1.75 mm filament. Some older or professional printers use 2.85 mm (often sold as “3 mm”).
- If the profile says 1.75 mm on a printer that really uses 2.85 mm filament, the printer feeds far more plastic than planned and badly over-extrudes. This usually happens with a hand-made or imported profile.
- Filament that runs thicker than its label also over-extrudes slightly. Good filament holds within a few hundredths of a millimetre.11The plastic delivered goes with the square of the diameter, so filament that is really 1.80 mm instead of 1.75 mm carries about 6% more plastic for every millimetre fed.
- If you suspect a spool, measure it with calipers in several places along a metre or so. Use the average in the slicer only if it’s consistently off.
Read the label: material, 1.75 mm diameter, 1 kg.Photo: John Abella from Outside Philadelphia, USA ·CC BY 2.0 ·Wikimedia Commons
A spool of white filament.Photo: Creative Tools ·CC BY 2.0 ·Wikimedia Commons
PLA: the beginner's filament.Photo: Richardspa ·CC0 ·Wikimedia Commons
Refill filament: a coil and a reusable spool.Photo: Suit ·CC BY-SA 4.0 ·Wikimedia Commons
Step 3: Check the nozzle size and line width
The slicer picks line widths from the nozzle size in the printer profile, usually around 100–120% of the nozzle diameter (about 0.42–0.48 mm for a 0.4 mm nozzle). If you swapped to a 0.4 mm nozzle but the profile still says 0.6 mm, the slicer plans 0.6–0.7 mm lines through a 0.4 mm hole. The plastic can’t spread that wide cleanly, so it piles up and looks over-extruded.
- Make sure the nozzle diameter in the printer profile matches the nozzle fitted. On Bambu printers the nozzle size is also chosen in the printer settings in Bambu Studio.
- Check line width settings haven’t been set much wider than the nozzle. Up to about 120% is normal; much more needs care.
A heater block in a silicone sock, with the nozzle below and heat break above.Photo: A7N8X ·CC0 ·Wikimedia Commons
The nozzle threads into the heater block.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
The mount that holds the hotend to the carriage.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
A brass 0.4 mm nozzle laying a thin strand.
Step 4: Calibrate the flow ratio
Once the big settings are right, the flow ratio fine-tunes the rest. Each filament, even each colour from one brand, flows a little differently, so this is set per filament.
- Most filaments land between 0.92 and 1.05. If you’re outside that, recheck steps 1–3 before going further.
- Change it in 2–5% steps when adjusting by eye, smaller steps once you’re close.
- OrcaSlicer and Bambu Studio have a built-in flow rate test in the Calibration menu. It prints a set of small patches with different flow values; pick the one with the smoothest top surface, with no gaps and no ridges.
- PrusaSlicer and Cura: print a single-wall cube in vase mode (Spiral vase in PrusaSlicer, Spiralize Outer Contour in Cura), measure the wall with calipers in several places, and set: new flow = old flow × line width ÷ measured wall.
- Or, more simply, print a 20 mm cube and look at the top surface. Gaps between lines: flow is low. Raised ridges and a rough, matte surface: flow is high. Flat, slightly glossy lines that just touch: about right.
A printed bowl: walls only, no infill.Photo: Sumanbargavr ·CC BY-SA 4.0 ·Wikimedia Commons
A twisted vase printed in a single wall.Photo: Sumanbargavr ·CC BY-SA 4.0 ·Wikimedia Commons
The calibration cube a few layers in.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
A screw-top box: threads print well at 0.2 mm layers.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
Where to find these settings in your slicer
| Setting | OrcaSlicer / Bambu Studio | PrusaSlicer | Cura |
|---|---|---|---|
| Flow ratio | Filament settings → Flow ratio | Filament Settings → Filament → Extrusion multiplier | Material → Flow |
| Filament diameter | Filament settings → Diameter | Filament Settings → Filament → Diameter | Material profile (Preferences → Materials) |
| Nozzle temperature | Filament settings → Nozzle temperature | Filament Settings → Filament → Temperature → Nozzle | Material → Printing Temperature |
| Nozzle diameter | Printer settings → Extruder → Nozzle diameter | Printer Settings → Extruder 1 → Nozzle diameter | Machine Settings → Extruder 1 → Nozzle size |
| Line width | Process → Quality → Line width | Print Settings → Advanced → Extrusion width | Quality → Line Width |
| Ironing | Process → Quality → Ironing | Print Settings → Infill → Ironing (Advanced or Expert mode) | Top/Bottom → Enable Ironing |
Menu names move between slicer versions. If you can’t find a setting, type its name into the slicer’s settings search box.
Step 5: Lower the nozzle temperature
Hotter plastic is runnier. It keeps oozing out of the nozzle during travel moves and while the head slows down at corners, leaving blobs, zits, droopy edges and strings. It doesn’t change how much filament the extruder pushes, but the result can look very like over-extrusion.
- If you’re at the top of the filament’s range, drop 5–10 °C and re-test.
- Stay inside the maker’s range. Too cold and you swap one problem for under-extrusion and weak layers.
| Filament | Typical nozzle range | Start at |
|---|---|---|
| PLA | 190–220 °C | 205 °C |
| PETG | 220–250 °C | 235 °C |
| TPU | 210–235 °C | 220 °C |
| ABS / ASA | 230–260 °C | 245 °C |
A temperature tower shows the whole range on one print; pick the coolest section that still has strong layers and clean walls. For material differences, see PLA vs PETG.
Hotter plastic is runnier: thinner, saggier strings.
0.8 mm of retraction: a few strings.
Ooze: a drop of molten plastic forming at the nozzle.Photo: David Elliott from UK ·CC BY 2.0 ·Wikimedia Commons
A thin strand pulled from the nozzle: where strings begin.Photo: David Elliott from UK ·CC BY 2.0 ·Wikimedia Commons
Step 6: Check the first layer
If only the bottom of the print looks over-extruded, the problem is usually height, not flow. When the nozzle is too close to the bed, the first layer is squashed flat and pushed outwards. The bottom edge bulges, the first layer looks smeared or see-through-thin, and ridges form between lines.
- Raise the Z offset in 0.02–0.05 mm steps until first-layer lines are flat, touching and not smeared.
- Check the bed is level or the mesh is up to date, because a too-low corner over-squashes only there.
- If the bottom edge still flares out, read the elephant’s foot guide.
More on getting the height right: what is Z offset and how to level a 3D printer bed.
gap 0.20 mm · line 0.45 × 0.20 mm · good squish
- Drag ↕ raise / lower the nozzle
- ↑ ↓ one babystep, 0.02 mm (Shift: 0.10)
- 1 2 3 too high · good · too low
- Home back to 0.00
Z offset right: slightly squished lines that touch.
Too low: lines squashed thin, and the extruder struggles.
Cross-section, too low: the line is pressed into a sheet.
A first layer close up: lines pressed together on the bed.Photo: hdaniel ·CC BY-SA 2.0 ·Wikimedia Commons
A probed 5 × 5 mesh across the bed.
Nozzle height decides the first layer: too close, just right, too far.Photo: Stemfie3D ·CC BY-SA 4.0 ·Wikimedia Commons
Step 7: Calibrate the extruder steps
The firmware stores how far the extruder motor turns for each millimetre of filament: E-steps on Marlin printers, rotation_distance on Klipper. If that number is off, every filament over-extrudes by the same amount. Most printers ship correct, so check this mainly after fitting a new extruder, flashing new firmware or loading someone else’s config.
- Heat the nozzle to printing temperature.
- Mark the filament 120 mm above the extruder entry.
- Extrude 100 mm slowly (about 1–2 mm/s, so the hotend isn’t the limit).
- Measure from the entry to the mark. It should be 20 mm. Less than 20 mm left means it pushed more than 100 mm.
- New E-steps = old E-steps × 100 ÷ actual length extruded. On Marlin,
M503shows the current value,M92 E<value>sets it andM500saves it. On Klipper, new rotation_distance = old × actual ÷ 100, set in printer.cfg.
Many printers with closed firmware (Bambu, recent Prusa models) don’t expect you to change this. On those, leave the extruder alone and calibrate with flow ratio instead.
An extruder motor with its tension knob.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
An assembled extruder before it goes on the printer.Photo: John Abella ·CC BY 2.0 ·Wikimedia Commons
The mainboard: the printer's brain.Photo: kenming Wang ·CC BY-SA 2.0 ·Wikimedia Commons
Stepper drivers on the mainboard, one per motor.Photo: kenming Wang ·CC BY-SA 2.0 ·Wikimedia Commons
Step 8: Tune pressure advance
Molten plastic in the nozzle is under pressure, and that pressure lags behind the motor. When the print head slows down for a corner, the pressure is still high, so extra plastic squeezes out and the corner bulges. When it stops at the end of a line, the leftover pressure leaves a blob.
Pressure advance (called Linear Advance in Marlin, and part of flow dynamics calibration on Bambu printers) fixes this by easing off the extruder just before the head slows down.
- If only corners and line ends look over-extruded while straight walls look fine, this is the likely cause.
- OrcaSlicer and Bambu Studio have a pressure advance (flow dynamics) test in the Calibration menu. Many Bambu printers can also run it automatically before a print.
- On Klipper it’s set in printer.cfg or by a G-code command; on Marlin with
M900 K<value>if the firmware has Linear Advance turned on. - On Klipper, values are small for direct drive (roughly 0.02–0.1) and higher for Bowden (roughly 0.3–1.0), because the long tube adds springiness. Marlin and other firmware use similar but not identical scales, so run the test rather than guessing. Too high thins out line starts and corners instead.
A print head at work over a plate of small parts.Photo: Neon Tommy ·CC BY-SA 2.0 ·Wikimedia Commons
A modern toolhead: extruder, hotend and fans in one housing.Photo: disinterpreter ·CC BY-SA 2.0 ·Wikimedia Commons
An enclosed CoreXY printer on a home desk.Photo: Mortymore ·CC BY 2.0 ·Wikimedia Commons
Step 9: Fix a rough top surface
Sometimes walls look fine but the top surface is ridged, with raised edges between lines and a rough, matte finish. The nozzle then drags across those ridges on the next layer, which can make a scraping sound or knock tall, thin parts.
- Calibrate flow first (step 4). Top surfaces show over-extrusion before anything else does.
- Lower top-surface flow if your slicer has a separate setting (OrcaSlicer has a top surface flow ratio; Cura has Top/Bottom Flow). Try 95–98% of your normal flow.
- Use ironing for flat tops that must look good. The hot nozzle passes over the top layer again with a tiny bit of plastic, smoothing it. It adds print time, so use it only where it matters.
Useful prints: planters on a shelf.Photo: Aaaatu ·CC BY-SA 4.0 ·Wikimedia Commons
A part being printed on a spring-steel bed.Photo: Leonhard Lenz ·CC BY-SA 4.0 ·Wikimedia Commons
Benchy cut open: walls, infill and overhangs in one small boat.Photo: CreativeTools: https://www.thingiverse.com/Cr… ·CC0 ·Wikimedia Commons
Step 10: Fix tight holes and oversized parts
Even with correct flow, plastic spreads a little as it’s laid, so outer edges sit slightly outside the planned line and holes come out slightly smaller than drawn. That’s normal and isn’t fixed by lowering flow. Turning flow down until holes fit would leave the rest of the part under-extruded.
Use the slicer’s size compensation instead:
- Cura: Horizontal Expansion (whole part) and Hole Horizontal Expansion (holes only).
- PrusaSlicer: XY Size Compensation.
- OrcaSlicer / Bambu Studio: X-Y hole compensation and X-Y contour compensation.
Start small: 0.05–0.15 mm of hole expansion, or a negative contour value of about the same size if the outside is too big. Re-print and measure. For parts that must fit together, design in a gap of about 0.2–0.3 mm between them as well.
Settings by material
| Material | Over-extrusion risk | Nozzle | Watch out for |
|---|---|---|---|
| PLA | Low | 190–220 °C | Printing near the top of the range, which oozes and blobs |
| PETG | High | 220–250 °C | Sticky, ooze-prone; often needs flow a few percent below PLA, and slower top layers |
| TPU | Medium | 210–235 °C | Oozes on travel; keep speed low and flow at the profile value |
| ABS / ASA | Medium | 230–260 °C | Shrinks as it cools, so size errors can be shrinkage rather than flow |
Start from the maker’s profile for the exact filament, then calibrate flow for each new spool type.
PLA: the beginner's filament.Photo: Richardspa ·CC0 ·Wikimedia Commons
A 1 kg spool of PETG, sealed with desiccant.Photo: Suit ·CC BY-SA 4.0 ·Wikimedia Commons
Flexible filament: label shows its print temperature.Photo: Sweetclara ·CC BY-SA 4.0 ·Wikimedia Commons
A spool of ABS.Photo: Tatár Lehel ·CC BY-SA 3.0 ·Wikimedia Commons
When over-extrusion won’t go away
If you’ve worked through every step:
- Reset to the stock profile for your printer and filament, and change one thing at a time.
- Try a fresh spool from another brand, to rule out filament that’s thicker than labelled.
- Check the thermistor reading. If the nozzle is actually hotter than the screen says, the plastic oozes like it’s overheated. A loose thermistor or a wrong sensor type in the firmware can cause this.
- Check for a leaking hotend. Plastic leaking between the nozzle and heater block can drip onto the print and look like blobs. Tighten the nozzle hot, following your printer’s manual.
The "blob of death": plastic that leaked and wrapped the hotend.Photo: LunaEatsTuna ·CC BY-SA 4.0 ·Wikimedia Commons
The heater block holds the heater cartridge and the thermistor.
A hotend being built: the heater wrapped in Kapton tape.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
Your action plan
- Undo recent flow increases and check the printer’s screen for a flow override.
- Confirm 1.75 mm (or 2.85 mm) filament diameter in the slicer.
- Match the nozzle size in the profile to the nozzle fitted.
- Calibrate the flow ratio for this filament.
- Lower the temperature 5–10 °C if you’re at the top of the range.
- Raise the Z offset if only the first layer is squashed.
- Calibrate E-steps if you changed the extruder or firmware.
- Tune pressure advance for bulging corners.
- Use hole and XY compensation for fit, not flow.
FAQ
What does over-extrusion look like?
Rough or lumpy walls, blobs and zits, ridged top surfaces, parts that measure slightly too big and holes that are too small. In bad cases the nozzle drags through the top layers and you hear it scraping.
Is over-extrusion or under-extrusion worse?
Neither is good, but slight over-extrusion usually gives stronger, if uglier, parts, while under-extrusion leaves gaps and weak layers. Aim for the flow where lines just touch with no gaps and no ridges.
What flow ratio should I use?
Most filaments end up between 0.92 and 1.05 (92–105%). Start from the maker’s profile, then run a flow calibration. If you need a value well outside that range, check filament diameter, nozzle size and E-steps first.
Can temperature cause over-extrusion?
Not directly, because the extruder pushes the same length either way. But a nozzle that’s too hot makes runny plastic that oozes during travel and at corners, which looks the same. Try 5–10 °C cooler if you’re at the top of the range.
Why are my holes too small if my flow is right?
Plastic spreads slightly as it’s laid, and curved holes are printed as many short straight lines, so holes almost always come out a little small. Use your slicer’s hole compensation instead of lowering flow.
Related guides
If you over-corrected and now see gaps, read under-extrusion. For bulging bottom layers, see elephant’s foot, and for hairs between parts, how to fix stringing. To understand the extruder and hotend involved, read parts of a 3D printer explained, and to find each setting, how to use a slicer. New to printing? Start with the complete beginner’s guide.