Nozzle School · Troubleshooting
Poor Overhangs in 3D Printing: Why They Curl and Droop, and Fixes
Why 3D printed overhangs curl up, droop or turn rough, and how to fix them with cooling, speed, temperature, layer height, part orientation and supports.
Poor overhangs are faces that lean outwards and print badly: the edges curl up, the lines droop and sag, or the underside comes out rough and stringy. It happens because each new line has less of the line below to rest on as the angle gets steeper, so it hangs partly in the air while it’s still soft. You fix it by cooling the plastic faster (more part-cooling fan), printing those areas slower and a little cooler, using thinner layers, turning the part so steep faces lean less, and adding supports for anything past about 45–60°.
This guide explains why overhangs fail, how to tell curling from drooping and from other faults, and what to change in OrcaSlicer, Bambu Studio, PrusaSlicer and Cura. It works on any FDM printer.
Quick fix checklist
Work down the list and re-print the same part, or an overhang test, after each change:
- Check the part-cooling fan runs and blows at the nozzle tip, not above it.
- Turn cooling up on overhangs: 100 % for PLA, more than your normal setting for PETG and ABS.
- Slow down overhanging walls to roughly 10–30 mm/s for the steepest sections.
- Lower the nozzle temperature by 5–10 °C if you’re near the top of the filament’s range.
- Use a thinner layer height (0.12–0.16 mm) for parts with steep overhangs.
- Calibrate flow: over-extruded overhang lines droop and curl more.
- Turn the part so steep faces lean less, or split it into pieces.
- Add supports for anything steeper than about 50–60° from vertical, and for flat ceilings.
The hull is a curved overhang test.Photo: CreativeTools: https://www.thingiverse.com/Cr… ·CC0 ·Wikimedia Commons
3DBenchy, the test model every printer is judged by.Photo: Creative Tools ·CC BY 2.0 ·Wikimedia Commons
Why supports exist: a sphere needs something under it.Photo: Mr N ·CC BY-SA 4.0 ·Wikimedia Commons
The hotend fan cools the heatsink. It must run whenever the hotend is hot.
A small fan cooling the extruder assembly.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
A print head at work over a plate of small parts.Photo: Neon Tommy ·CC BY-SA 2.0 ·Wikimedia Commons
What is an overhang?
An overhang is any part of a model that leans out past the layer below it. Think of the underside of a chin on a figurine, the curved hull of a boat, the top half of a round hole, or a shelf sticking out of a wall.
Overhangs are measured as an angle from vertical:
- 0° is a straight vertical wall. Every layer sits exactly on the one below.
- 45° leans out halfway between vertical and flat. Most printers handle this without help.
- 60–70° is steep. Some printers manage it with good cooling, many show droop and curling.
- 90° is flat, a horizontal ceiling with nothing under it. That’s not an overhang the printer can build up gradually; it has to bridge between supports or use support material.11Slicers don’t all count the same way. Cura’s support overhang angle counts from vertical, like this guide. OrcaSlicer, Bambu Studio and PrusaSlicer set the support threshold as the face’s slope from horizontal, so 30° there means the same as 60° here. 45° is the same either way.
A related idea is the overhang percentage that OrcaSlicer and Bambu Studio show: how much of a line’s width hangs out past the line below. 0 % is fully supported, 100 % is fully in the air.
What poor overhangs look like
- Curling up: the outer edge of the overhang lifts and bends upwards, making a ragged lip. You may hear the nozzle tick or scrape as it hits the curled edge on the next layer.
- Drooping or sagging: lines hang down below where they should be, so the underside looks wavy, stringy or “melted”.
- A rough, ridged underside, with loose loops of plastic, even though the top side looks fine.
- Gaps between the outer wall and the inner walls on the overhanging side.
- The overhang gets worse with height: it starts fine and falls apart as the angle builds up.
- Small features, like the top of a round hole or a chin, come out flattened or blobby.
Printed Benchys in different filaments.Photo: 3DBenchy ·CC BY 2.0 ·Wikimedia Commons
Another failed Benchy: messy, sagging layers.Photo: 3DBenchy ·CC BY 2.0 ·Wikimedia Commons
A dual-extrusion Benchy gone wrong.Photo: 3DBenchy ·CC BY 2.0 ·Wikimedia Commons
Test prints on the way from failure to a clean part.Photo: Dbsnp ·CC BY-SA 4.0 ·Wikimedia Commons
Poor overhangs and faults that look similar
- Warping: corners of the part lift off the bed. That’s the whole part shrinking as it cools, not an overhang problem, though the cause (uneven cooling and shrinkage) is related. See how to fix warping.
- Sagging bridges: a flat span between two supports droops in the middle. Bridges follow similar rules but have their own settings; see the bridge note in step 9.
- Stringing: thin hairs between separate parts of a print, from oozing during travel moves. See how to fix stringing.
- Rough support scars: the underside is rough because supports were torn off, not because the overhang failed. That’s a support interface and gap problem (step 8).
- Over-extrusion everywhere: lumpy walls on every side, not just the leaning ones. See over-extrusion.
- Layer shift: a sharp sideways step at one height. Sometimes caused by the nozzle hitting a curled overhang, so fix the overhang first. See layer shifting.
Why overhangs fail
Each line needs something to sit on
Your printer lays plastic as a flattened line, typically about 0.45 mm wide and 0.2 mm tall from a 0.4 mm nozzle. On a vertical wall, each new line sits squarely on the one below. On an overhang, each layer is shifted outwards a little, so part of the new line rests on the line below and part hangs in the air.
How much hangs out depends on the angle and the layer height. Each layer steps out by layer height × tan(angle):
| Overhang angle | Step out per 0.2 mm layer | Share of a 0.45 mm line still supported |
|---|---|---|
| 30° | 0.12 mm | About 75 % |
| 45° | 0.20 mm | About 55 % |
| 55° | 0.29 mm | About 37 % |
| 60° | 0.35 mm | About 23 % |
| 65° | 0.43 mm | About 5 % |
| 70° | 0.55 mm | None |
That’s why 45° is the usual rule of thumb: about half of each line still sits on solid plastic, which is enough to hold it while it cools. Past about 55–60°, most of the line is in the air, and only cooling and the stiffness of the plastic hold it up.22The table is simple geometry for a rectangular line. Real lines are rounded, and the slicer may widen or reorder walls on overhangs, so treat the numbers as a guide to the trend, not exact limits.
Hot plastic droops, cooling plastic curls
The unsupported part of the line is soft for a moment after it leaves the nozzle. If it stays soft too long, gravity and the drag of the nozzle pull it down: that’s droop.
If it cools fast on top but the plastic shrinks as it cools, the edge can bend up instead: the freshly laid line shrinks onto a layer that has already shrunk, and the thin, unsupported edge has nothing holding it flat. That’s curling. Curled edges then stick up into the nozzle’s path on the next layer, and each layer makes it worse.
So overhangs depend on how quickly the line sets:
- Cooling (part-cooling fan) sets it faster.
- Speed gives the fan more or less time per millimetre of line, and slower overhang lines are pulled less by the nozzle.
- Temperature: cooler plastic is stiffer and sets sooner.
- Layer height: thinner layers step out less per layer, so more of each line is supported.
- Flow: extra plastic on an overhang is extra weight hanging in the air.
overhang 45° · line 56 % held · fan 100 % · droop 0.00 mm
- O B overhang wall / bridge (or click either)
- ← → wall angle ±5° (0–70°) or bridge span ±5 mm (10–60 mm); or drag ↔
- ↑ ↓ part-cooling fan ±10 %
- T nozzle temperature: 200 / 215 / 230 °C (PLA)
- Home reset: 45° wall, fan 100 %, 215 °C
30° from vertical: overhang 30° · line 74 % held · fan 100 % · droop 0.00 mm
45° from vertical: overhang 45° · line 56 % held · fan 100 % · droop 0.00 mm
60° from vertical: overhang 60° · line 23 % held · fan 100 % · droop 0.10 mm

Solid filament above the heat break, molten filament in the heater block.
A brass 0.4 mm nozzle laying a thin strand.
The print head: extruder on top, finned heatsink, heater block and nozzle.
Cause and fix reference
| What you see | Most likely cause | Fix | Step |
|---|---|---|---|
| Overhang edges curl up, bad on all filaments | Weak or misaimed part-cooling | Check the fan and duct | 1 |
| Droop and curl on PLA with fan below 100 % | Not enough cooling on overhangs | Raise overhang fan speed | 2 |
| Underside rough, lines dragged and looped | Overhang printed too fast | Slow down overhangs | 3 |
| Glossy, saggy overhangs, some stringing | Nozzle too hot | Lower temperature 5–10 °C | 4 |
| Fine below 45°, falls apart past 50–55° | Layers step out too far | Thinner layers | 5 |
| Thick, heavy, blobby overhang edges | Over-extrusion | Calibrate flow | 6 |
| Steep faces fail whatever you change | Geometry | Re-orient, split, chamfer | 7 |
| Angles past about 60°, flat ceilings | Beyond what can print unsupported | Add supports | 8 |
| Curling only on small, thin or tall parts | Each layer prints too quickly to cool | Minimum layer time, print copies | 9 |
Step 1: Check the part-cooling fan
Start here, because no setting helps if the air isn’t getting there. Every FDM toolhead has two kinds of fan:
- The hotend fan cools the heatsink so filament doesn’t melt too high up. It runs all the time the hotend is hot.
- The part-cooling fan blows through a duct at the plastic just after it leaves the nozzle. That’s the one overhangs need. The slicer turns it up and down.
What to check:
- Start a print and watch the part-cooling fan come on after the first layer or two. If it doesn’t spin, or spins slowly, check the wiring and the fan for dust or hair.
- Look at where the duct points. The air should hit the plastic just below and around the nozzle tip, not the heater block and not far below. A cracked, melted or bent duct sends air the wrong way.
- Check whether the air reaches the side of the part where the overhang is. Single-sided ducts cool one side better than the other, so an overhang facing away from the fan curls more. If yours does that, try rotating the part in the slicer so the overhang faces the fan.
- Make sure a silicone sock (if fitted) is in place on the heater block, so the fan cools the plastic and not the heater.
The hotend fan cools the heatsink. It must run whenever the hotend is hot.
A small fan cooling the extruder assembly.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
A modern toolhead: extruder, hotend and fans in one housing.Photo: disinterpreter ·CC BY-SA 2.0 ·Wikimedia Commons
A dual-nozzle head: two hotends side by side.Photo: Creative Tools from Halmstad, Sweden ·CC BY 2.0 ·Wikimedia Commons
Step 2: Turn up cooling on overhangs
Most slicers set the fan from the filament profile, and let you raise it automatically for overhangs and bridges.
- PLA: run the part-cooling fan at 100 % after the first few layers. PLA can almost always take full cooling, and overhangs benefit most.
- PETG: normal fan is lower, often 30–60 %, because too much cooling weakens layer bonds. Raise overhangs and bridges to 70–100 % with the overhang fan setting rather than raising the whole print.
- ABS and ASA: usually printed with 0–30 % fan to avoid cracking and warping. Raise overhangs to around 30–60 %, in an enclosure, and lean more on slower speeds and supports.
- TPU: moderate fan, around 30–60 %; it’s soft and floppy, so supports help more than cooling.
The overhang fan settings let you do this only where it’s needed, so the rest of the print keeps its normal cooling and layer strength.
ABS · bed 100 °C · open air · corner lift 0.80 mm · warping
- M material: PLA or ABS (or click the controller screen)
- E enclosure on / off (or click the frame)
- F fan draft on / off (or click the fan)
- B brim on / off (or click the print)
- ↑ ↓ bed temperature ±5 °C (Shift ±10), 20–115 °C; or drag ↕
- Home reset: ABS, bed 100 °C, open air, no brim
ABS, bed 100 °C, open air: ABS · bed 100 °C · open air · corner lift 0.80 mm · warping.
ABS in a draft: ABS · bed 100 °C · fan draft · corner lift 1.17 mm · warping.
ABS in an enclosure: ABS · bed 100 °C · enclosed · corner lift 0.28 mm · slight lift.
Step 3: Slow down overhanging walls
Speed matters in two ways. A slower line gives the fan more time per millimetre to cool it, and the nozzle tugs less on a soft line that’s only half supported.
Most slicers can slow down only the overhanging parts of a wall:
- OrcaSlicer and Bambu Studio sort overhangs into bands by how much of the line hangs out (10 %, 25 %, 50 %, 75 % and, in Bambu Studio, 100 %) and let you set a speed for each. Typical values run from around 30–50 mm/s for mild overhangs down to 10–20 mm/s for the steepest.
- PrusaSlicer has dynamic overhang speed (Expert mode), which works the same way with speeds for 0 %, 25 %, 50 % and 75 % overlap.
- Cura has Overhanging Wall Angle and Overhanging Wall Speeds in its Experimental section, which slow walls past that angle to a percentage of the normal wall speed.
If your slicer doesn’t do it automatically, a simple fix is to lower the outer wall speed to around 25–40 mm/s for prints with tricky overhangs.
An enclosed CoreXY printer on a home desk.Photo: Mortymore ·CC BY 2.0 ·Wikimedia Commons
A CoreXY print head on a QIDI printer.Photo: Haroldbarlow8911 ·CC BY-SA 4.0 ·Wikimedia Commons
An assembled Ender 3: a classic bed-slinger.Photo: kenming Wang ·CC BY-SA 2.0 ·Wikimedia Commons
Step 4: Lower the nozzle temperature
Hotter plastic is runnier and takes longer to set, so it droops more on overhangs. If you’re printing near the top of the filament’s range:
- Lower the nozzle temperature by 5–10 °C and re-test.
- Stay inside the filament’s range. Too cold and layers bond poorly, so the overhang may hold its shape but break off easily.
A temperature tower shows the trade-off in one print: most towers include an overhang on every block, so you can see where it starts to droop. See how to print a temperature tower.
210 °C · 1 string · overhang sag 0.2 mm · bridge droop 0.2 mm · satin · layers 99 % · good
- ↑ ↓ next block up (cooler) or down (hotter); or click a block
- Home End bottom (230 °C) or top (190 °C)
- B the pick: the coolest strong, clean block (205 °C here)
195 °C, 0.8 mm retraction: few strings.
210 °C, 0.8 mm retraction: few strings.
225 °C, 0.8 mm retraction: many strings.
Ooze: a drop of molten plastic forming at the nozzle.Photo: David Elliott from UK ·CC BY 2.0 ·Wikimedia Commons
Step 5: Use thinner layers
The table earlier shows why: each layer steps out by layer height × tan(angle). Halve the layer height and each line steps out half as far, so more of it sits on the line below.
| Layer height | Step out at 60° | Share of a 0.45 mm line supported |
|---|---|---|
| 0.28 mm | 0.48 mm | None |
| 0.20 mm | 0.35 mm | About 23 % |
| 0.16 mm | 0.28 mm | About 38 % |
| 0.12 mm | 0.21 mm | About 54 % |
So a 60° overhang that fails at 0.2 mm often prints at 0.12 mm. The cost is print time. Many slicers let you use thinner layers only where they’re needed (variable layer height or adaptive layers), which keeps the time down. For more on picking a height, see layer height explained.
Layer 25 of 225, z 5.0 mm.
Layer 100 of 225, z 20.0 mm.
Layer 200 of 225, z 40.0 mm.
Step 6: Check flow and wall settings
Flow: too much plastic makes overhang lines thicker and heavier, so they droop, and the extra plastic piles up at the edge and curls. Calibrate flow for each filament; see flow rate calibration. If walls look lumpy everywhere, see over-extrusion.
Wall order: most slicers print the inner walls first, then the outer wall. On an overhang, that means the outer wall leans against an inner wall that was just printed, which supports it. If you’ve switched to outer wall first for better dimensional accuracy, overhangs usually get worse. Switch back for parts with steep overhangs.
Overhang tools in the slicer:
- Detect overhang walls (OrcaSlicer) or detect bridging perimeters (PrusaSlicer) lets the slicer treat steep overhanging walls specially, with bridge-like flow, speed and fan.
- Extra perimeters on overhangs (OrcaSlicer, PrusaSlicer) adds walls under steep overhangs so the outer wall has something to lean on.
- Reverse on even (OrcaSlicer) prints overhanging walls in alternating directions on odd and even layers, which helps stop curling on steep overhangs.
- Make overhangs printable (OrcaSlicer, and Cura’s experimental Make Overhang Printable) changes the model’s shape under steep overhangs into a printable cone, which saves supports but changes how the part looks underneath.
Try one at a time and re-print the same part, so you know what helped.
flow 1.00 · 1.75 mm filament · asks 0.45 · lays 0.45 mm · flat, touching
- Drag ↔ flow ratio
- ← → flow ±0.01 (Shift ±0.05), 0.85–1.15
- ↑ ↓ filament diameter ±0.01 mm, 1.70–1.80
- 1 2 3 too low · right · too high
- Home reset: 1.00 on 1.75 mm
Step 7: Orient and design for overhangs
Often the best overhang fix is to not print it as an overhang.
- Turn the part in the slicer so steep faces lean less, or face up. A bracket printed lying on its side may have no overhangs at all.
- Split the part into two pieces that each print flat, then glue or bolt them together.
- Put the best face on top or on the sides. Undersides are always a little rougher.
- Face overhangs towards the fan if your printer cools one side better.
If you design your own parts:
- Use 45° chamfers instead of flat ledges. A chamfer prints cleanly; a flat ledge needs support.
- Make horizontal holes teardrop-shaped, with a 45° point at the top, so the top of the hole isn’t a flat bridge.
- Use fillets and curves on the underside sparingly. The bottom of a curve starts at nearly 90° and is the hardest part to print.
- Keep unsupported overhangs at or below 45–50° if they must print without supports.
A working wrench printed in one piece.Photo: Creative Tools from Halmdstad, Sweden ·CC BY 2.0 ·Wikimedia Commons
A screw-top box: threads print well at 0.2 mm layers.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
A printed maze puzzle.Photo: Sumanbargavr ·CC BY-SA 4.0 ·Wikimedia Commons
A table of small prints.Photo: Trevor Prentice ·CC BY-SA 2.0 ·Wikimedia Commons
Step 8: Add supports where they are needed
Past about 55–60° from vertical, or for any flat ceiling, the plastic needs something underneath. That’s what supports are for: the slicer builds a scaffold under the overhang that you break off after printing.
Key settings:
- Overhang (threshold) angle: the steepest face the slicer will print without support. Counted from vertical, as in Cura, 45–55° is a common starting point; raise it towards 60° if your printer handles overhangs well. In OrcaSlicer, Bambu Studio and PrusaSlicer the threshold counts from horizontal (note 1), so the same range is about 35–45°, and a lower number there means fewer supports.
- Normal vs tree supports: normal (grid) supports are blocks straight down; tree supports branch up from a few points and touch the part only where needed, using less plastic and leaving fewer marks on curved parts.
- Top Z distance: the small gap between the support’s top and the part, usually around 0.1–0.3 mm (often one layer height). Bigger gaps peel off more easily but leave a rougher underside; smaller gaps give a smoother underside but fuse more.
- Interface layers: a few denser layers at the top of the support give the overhang a flatter surface to print on.
- Support on build plate only: stops supports growing on top of the part itself, which is easier to clean up.
Supports hold up overhangs while the print grows.Photo: Nevit ·CC BY-SA 3.0 ·Wikimedia Commons
Why supports exist: a sphere needs something under it.Photo: Mr N ·CC BY-SA 4.0 ·Wikimedia Commons
Gyroid infill in a slicer preview.Photo: Anachronist ·CC BY-SA 4.0 ·Wikimedia Commons
Where to find these settings in your slicer
| Setting | OrcaSlicer / Bambu Studio | PrusaSlicer | Cura |
|---|---|---|---|
| Part-cooling fan | Filament settings → Cooling → Part cooling fan → Min and Max fan speed threshold | Filament Settings → Cooling → Fan settings → Fan speed (Expert mode) | Cooling → Regular Fan Speed and Maximum Fan Speed |
| Overhang fan | Filament settings → Cooling → Overhangs and external bridges fan speed (Bambu Studio: Fan speed for overhang), with Force cooling for overhangs and bridges | Filament Settings → Cooling → Enable dynamic fan speeds (Expert mode) | No separate overhang fan; Experimental → Bridge Fan Speed covers bridges |
| Overhang speed | Process → Speed → Slow down for overhangs, then the Overhang speed boxes (10 %, 25 %, 50 %, 75 %) | Print Settings → Speed → Dynamic overhang speed (Expert mode) | Experimental → Overhanging Wall Angle and Overhanging Wall Speeds |
| Outer wall speed | Process → Speed → Outer wall | Print Settings → Speed → External perimeters | Speed → Outer Wall Speed |
| Layer height | Process → Quality → Layer height | Print Settings → Layers and perimeters → Layer height | Quality → Layer Height |
| Wall order | OrcaSlicer: Process → Quality → Walls and surfaces → Walls printing order | Print Settings → Layers and perimeters → External perimeters first (leave it off) | Walls → Wall Ordering |
| Overhang tools | OrcaSlicer: Process → Quality → Overhangs (Detect overhang walls, Make overhangs printable, Extra perimeters on overhangs, Reverse on even); not in Bambu Studio | Print Settings → Layers and perimeters → Detect bridging perimeters, Extra perimeters on overhangs (Expert mode) | Experimental → Make Overhang Printable |
| Supports | Process → Support → Enable support, Type, Threshold angle; Top Z distance under Support → Advanced | Print Settings → Support material → Generate support material, Overhang threshold, Top contact Z distance | Support → Generate Support, Support Structure, Support Overhang Angle, Support Top Distance |
Many of these only show once you switch the slicer to its Advanced or Expert view. Menu names also move between versions, so if you can’t find a setting, type its name into the settings search box. If you’re new to the menus, start with how to use a slicer.
Step 9: Give small layers time to cool
On a small or thin part, each layer takes only a few seconds, so the nozzle comes back before the last layer has cooled. Overhangs on small parts (the tip of a horn, a thin arm) curl and droop even with good settings for larger parts.
- Check the minimum layer time (OrcaSlicer and Bambu Studio call it “slow printing down for better layer cooling”). Around 5–10 seconds suits PLA; the slicer slows down small layers to reach it.
- Print two or more copies, or add a second small object, so each layer takes longer.
- Let the fan run at full speed on small layers; most profiles do this automatically.
Bridges are the flat cousin of overhangs: a line printed across open air between two supports. They use their own speed, flow and fan settings, and fail by sagging in the middle. The same rules apply (cool hard, don’t print too hot), and the bridge settings are the place to tune them.
Settings by material
| Material | Nozzle | Normal fan | Overhang fan | Notes |
|---|---|---|---|---|
| PLA | 190–220 °C | 100 % (after layer 2–3) | 100 % | The easiest; most PLA manages 45–60° with good cooling |
| PETG | 220–250 °C | 30–60 % | 70–100 % | Droops and strings more; slow overhangs and lower temperature help most |
| ABS / ASA | 230–260 °C | 0–30 % | 30–60 % | Curls easily; print enclosed, slow, and support steep faces |
| TPU | 210–235 °C | 30–60 % | 50–100 % | Soft and floppy; prefer supports and slow speeds |
These are starting points. Begin from the maker’s profile for your exact filament, then adjust overhang fan and speed.
PLA: the beginner's filament.Photo: Richardspa ·CC0 ·Wikimedia Commons
A 1 kg spool of PETG, sealed with desiccant.Photo: Suit ·CC BY-SA 4.0 ·Wikimedia Commons
A spool of ABS.Photo: Tatár Lehel ·CC BY-SA 3.0 ·Wikimedia Commons
Flexible filament: label shows its print temperature.Photo: Sweetclara ·CC BY-SA 4.0 ·Wikimedia Commons
When overhangs still won’t print
If you’ve worked through every step:
- Print an overhang test (many free models step from 20° to 70° in 5° or 10° steps) to see exactly where your printer starts to fail. Then set the support threshold just below that angle.
- Upgrade the part-cooling duct or fan if your printer has a small single-sided fan. Many printers have well-tested replacement ducts; use one designed for your exact toolhead.
- Dry the filament. Wet filament oozes and bubbles, which makes overhangs rough and stringy. See how to dry filament.
- Check for drafts and room temperature. A cold draft cools one side unevenly; a hot enclosure with PLA can slow cooling so much that overhangs droop. Open the door of an enclosure for PLA.
- Reset to the stock profile and change one setting at a time.
An enclosure keeps heat in for ABS and ASA.Photo: -stk ·CC BY-SA 4.0 ·Wikimedia Commons
An open spool of PLA left out in the air.Photo: SuperBlobMonster ·CC BY-SA 3.0 ·Wikimedia Commons
A 20 mm calibration cube, often the first print.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
Your action plan
- Check the part-cooling fan runs and its duct aims at the nozzle tip.
- Raise overhang cooling: 100 % for PLA, overhang fan up for PETG and ABS.
- Slow down overhanging walls, or the outer wall, to 10–30 mm/s at the steepest.
- Lower the nozzle 5–10 °C if you’re near the top of the range.
- Use 0.12–0.16 mm layers for steep overhangs, or variable layer height.
- Calibrate flow and print inner walls before outer walls.
- Re-orient the part, split it, or add 45° chamfers to your own designs.
- Add supports for faces steeper than about 55–60° and for flat ceilings.
FAQ
What is the maximum overhang angle for 3D printing?
Most printers handle 45° from vertical without help, and many manage 55–60° with good cooling, slow overhang speeds and thin layers. Past about 60–70°, nearly all of each line hangs in the air, so you need supports.
Why do my overhangs curl up?
The thin, unsupported edge cools and shrinks with nothing holding it flat, so it bends upwards. More cooling, slower overhang speeds and a slightly lower temperature help. Curling is worse on ABS and ASA, which shrink more, and on parts facing away from a single-sided fan.
Does a lower layer height help overhangs?
Yes. Each layer steps out by the layer height times the tangent of the angle, so thinner layers lean out less and more of each line rests on the one below. A 60° overhang that fails at 0.2 mm often prints at 0.12 mm.
Should I use supports or fix the settings?
Both, in that order. Tune cooling, speed and temperature first so your printer handles as steep an angle as it can, then set the support threshold just below that angle. You’ll use fewer supports and get cleaner parts.
Why are my overhangs worse on one side of the part?
Your part-cooling fan probably blows from one side. Overhangs facing the fan get more air than ones facing away. Rotate the part in the slicer so the worst overhang faces the fan, or fit a duct that blows from both sides.
Do overhangs need 100 % fan?
For PLA, yes, it almost always helps. For PETG, ABS and ASA, full fan everywhere can weaken layers and cause cracks, so use the overhang fan setting to raise cooling only on overhangs.
Related guides
Overhangs share a cause with warping: plastic shrinking as it cools. To find your filament’s best temperature, print a temperature tower, and to dial in plastic flow, see flow rate calibration. If a curled overhang knocked your print sideways, read layer shifting, and for ridges up the walls rather than at overhangs, see Z banding. New to printing? Start with the complete beginner’s guide.