Why 3D prints warp and corners lift off the bed, and how to stop it step by step: bed prep, temperature, brims, cooling, enclosures and part design.
Warping is when the corners or edges of a print curl up off the bed, because plastic shrinks as it cools and the lower layers get pulled upwards by the layers above them. You fix it by giving the first layer a clean, well-adjusted bed to grip, keeping the print warm and out of drafts, and adding a brim on parts that still lift.
This guide covers every cause we know of, how to tell warping apart from faults that look similar, and the settings to change in OrcaSlicer, Bambu Studio, PrusaSlicer and Cura. It works for any FDM printer.
Quick fix checklist
Work down this list and re-print after each change:
- Clean the build plate with isopropyl alcohol, or dish soap and water for PEI sheets.
- Check the first layer: it should be slightly squished, with lines that touch.
- Use the right bed temperature for your filament.
- Add a brim (5–10 mm) to wide, flat parts and parts with sharp corners.
- Turn the part cooling fan off for the first few layers.
- Keep drafts away: close windows, move the printer away from fans and air conditioning, or use an enclosure.
- Round sharp corners and lay parts so the smallest footprint possible sits on the bed.
The heated bed with a PEI sheet. The part is the only thing printed on it.
A first layer close up: lines pressed together on the bed.Photo: hdaniel ·CC BY-SA 2.0 ·Wikimedia Commons
The first layers going down on a heated bed.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
An enclosure keeps heat in for ABS and ASA.Photo: -stk ·CC BY-SA 4.0 ·Wikimedia Commons
A print on a glass bed.Photo: ENERGY.GOV ·Public domain ·Wikimedia Commons
A scraper: lift prints off a rigid bed.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
What is warping?
Warping is a print bending out of shape as it cools. It usually shows up as corners lifting off the bed on wide, flat parts, but it can also show as a part that rocks on a table, a bottom that isn’t flat, or cracks between layers higher up.
It happens because almost all plastics shrink as they cool. Each new layer goes down hot and shrinks on top of the cooler layer below it. That pulls the edges inwards and upwards, and the corners, where the pull comes from two directions, are first to let go of the bed.11ABS and ASA shrink noticeably more than PLA as they cool, which is why they warp so much more easily and usually need an enclosure.
Warping, poor adhesion, curling and splitting look similar
- Warping: the print stays stuck in the middle, but the corners and edges lift, often after many layers. Usually worse on big, flat parts.
- Poor first-layer adhesion: the very first layer never sticks properly, so lines drag around or the whole part comes loose early. That’s a bed and Z offset problem; see first layer not sticking.
- Curling overhangs: edges of overhangs lift up in the air as they print, nowhere near the bed. That’s a cooling and overhang problem, not warping.
- Layer splitting: cracks appear between layers higher up the part, especially on ABS. It has the same root cause as warping (shrinking plastic), but it shows up as cracks instead of lifted corners.
A print that broke loose partway through.Photo: EwkaC ·CC BY-SA 4.0 ·Wikimedia Commons
The same failure from the side: layers stop where the part moved.Photo: EwkaC ·CC BY-SA 4.0 ·Wikimedia Commons
Spaghetti: the part came loose and the printer kept extruding into the air.Photo: SuperBlobMonster ·CC BY-SA 3.0 ·Wikimedia Commons
The hull is a curved overhang test.Photo: CreativeTools: https://www.thingiverse.com/Cr… ·CC0 ·Wikimedia Commons
Why supports exist: a sphere needs something under it.Photo: Mr N ·CC BY-SA 4.0 ·Wikimedia Commons
Nozzle height decides the first layer: too close, just right, too far.Photo: Stemfie3D ·CC BY-SA 4.0 ·Wikimedia Commons
Why warping happens
Three things decide whether a part warps:
- How much the plastic shrinks as it cools. ABS, ASA and nylon shrink a lot; PLA shrinks little.
- How hard the first layer grips the bed. A clean, warm, well-adjusted bed holds the corners down.
- How fast and unevenly the part cools. Drafts and strong cooling make the top shrink faster than the bottom can resist.
ABS · bed 100 °C · open air · corner lift 0.80 mm · warping
- M material: PLA or ABS (or click the controller screen)
- E enclosure on / off (or click the frame)
- F fan draft on / off (or click the fan)
- B brim on / off (or click the print)
- ↑ ↓ bed temperature ±5 °C (Shift ±10), 20–115 °C; or drag ↕
- Home reset: ABS, bed 100 °C, open air, no brim
A print bed in layers: heater, aluminium, magnet, spring steel, PEI.
The first few layers.
The control box shows nozzle and bed temperature, height and progress.
Layer 1 of 225, z 0.2 mm.
Layer 25 of 225, z 5.0 mm.
Layer 75 of 225, z 15.0 mm.
ABS, bed 100 °C, open air: ABS · bed 100 °C · open air · corner lift 0.80 mm · warping.
ABS, bed 100 °C, open air: ABS · bed 100 °C · open air · corner lift 0.80 mm · warping.
A dial gauge on the corner reads the lift: ABS · bed 100 °C · open air · corner lift 0.80 mm · warping.
The bed controller: actual temperature, setpoint and material.
PLA, bed 60 °C: PLA · bed 60 °C · open air · corner lift 0.00 mm · flat.
PLA on a cold bed: PLA · bed 20 °C · open air · corner lift 0.62 mm · warping.
Cause and fix reference
| What you see | Most likely cause | Fix | Step |
|---|---|---|---|
| Corners lift on a part that used to print fine | Dirty bed (finger oils, dust) | Clean the plate | 1 |
| First layer looks round and loose | Nozzle too high | Lower the Z offset | 3 |
| One side lifts, the other is fine | Bed not level | Level the bed | 3 |
| Corners lift after a few millimetres of height | Bed too cool, or fan too strong too early | Raise bed temp, delay the fan | 2, 5 |
| Long, flat parts curl at both ends | Shrinkage along the length | Brim or mouse ears | 4 |
| Warping only when a window or fan is on | Drafts | Block drafts, use an enclosure | 6 |
| ABS or ASA warps no matter what | High-shrink material without an enclosure | Enclosure, or switch material | 6, 7 |
| Sharp corners lift first, round parts are fine | Corner stress | Round corners, rotate the part | 8 |
Step 1: Clean the build plate
Try this first. Fingerprints leave oil on the plate, and oil stops the first layer gripping. Even a few touches while removing the last print are enough.
- Smooth or textured PEI: wipe with isopropyl alcohol (90% or more) before each print. Every so often, wash it with dish soap and warm water, then dry it.22Prusa recommends washing its PEI sheets with dish soap and warm water when isopropyl alcohol alone stops working.
- Glass: clean with isopropyl alcohol; many people add a thin layer of glue stick for PETG and ABS.
- Hold sheets by the edges, and don’t touch the print area.
A print on a glass bed.Photo: ENERGY.GOV ·Public domain ·Wikimedia Commons
A scraper: lift prints off a rigid bed.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
The heated bed with a PEI sheet. The part is the only thing printed on it.
A part being printed on a spring-steel bed.Photo: Leonhard Lenz ·CC BY-SA 4.0 ·Wikimedia Commons
A 20 mm calibration cube, often the first print.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
The calibration cube a few layers in.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
Step 2: Set the right bed temperature
A warm bed keeps the bottom layers soft and stuck down while the rest of the print shrinks above them. Too cool and they let go; much too hot and PLA can sag at the bottom (“elephant’s foot”).
Start with the filament maker’s recommended bed temperature, printed on the spool label or box, then adjust in 5 °C steps.
| Filament | Typical bed temperature |
|---|---|
| PLA | 55–65 °C |
| PETG | 70–85 °C |
| TPU | 40–60 °C |
| ABS / ASA | 95–110 °C |
Read the label: material, 1.75 mm diameter, 1 kg.Photo: John Abella from Outside Philadelphia, USA ·CC BY 2.0 ·Wikimedia Commons
PLA: the beginner's filament.Photo: Richardspa ·CC0 ·Wikimedia Commons
A 1 kg spool of PETG, sealed with desiccant.Photo: Suit ·CC BY-SA 4.0 ·Wikimedia Commons
A spool of ABS.Photo: Tatár Lehel ·CC BY-SA 3.0 ·Wikimedia Commons
ABS, bed 20 °C: ABS · bed 20 °C · open air · corner lift 1.56 mm · warping.
ABS, bed 40 °C: ABS · bed 40 °C · open air · corner lift 1.43 mm · warping.
ABS, bed 60 °C: ABS · bed 60 °C · open air · corner lift 1.29 mm · warping.
ABS, bed 80 °C: ABS · bed 80 °C · open air · corner lift 1.05 mm · warping.
ABS, bed 100 °C: ABS · bed 100 °C · open air · corner lift 0.80 mm · warping.
ABS, bed 110 °C: ABS · bed 110 °C · open air · corner lift 0.74 mm · warping.
Step 3: Get the first layer right
The first layer is what holds the corners down. If it’s too high, the lines are round and barely touch the bed; if the bed isn’t level, one side grips and the other doesn’t.
- Set the Z offset so the first layer is slightly squished and the lines touch. See what Z offset is and how to set it.
- Level the bed, or re-run auto leveling, so the gap is the same everywhere. See how to level a 3D printer bed.
- Print the first layer slower (20–30 mm/s is common) so it has time to bond.
gap 0.20 mm · line 0.45 × 0.20 mm · good squish
- Drag ↕ raise / lower the nozzle
- ↑ ↓ one babystep, 0.02 mm (Shift: 0.10)
- 1 2 3 too high · good · too low
- Home back to 0.00
Cross-section, too high: the line stays round.
Cross-section, right height: a flattened line, about 0.45 × 0.20 mm.
Cross-section, too low: the line is pressed into a sheet.
A probed 5 × 5 mesh across the bed.
A corner spring and knob: about half a millimetre per full turn.
Turn a knob and the old mesh no longer matches the bed. Probe again.
Step 4: Add a brim, mouse ears or a raft
A brim is a few loops of single-layer plastic printed around the bottom edge of the part. It gives the corners a much bigger area to grip, and you peel or trim it off afterwards.
- Brim: 5–10 mm wide works for most parts. Use it on wide, flat parts and anything with sharp corners.
- Mouse ears: small discs only at the corners, where warping starts. Less cleanup than a full brim.33OrcaSlicer and Bambu Studio offer brim “ears” as a brim type; in other slicers you can add small, thin cylinders at each corner yourself.
- Raft: a thick base printed under the whole part. It grips very well but wastes plastic and leaves a rough bottom. Save it for tough materials or very small contact areas.
The first layers going down on a heated bed.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
A first layer close up: lines pressed together on the bed.Photo: hdaniel ·CC BY-SA 2.0 ·Wikimedia Commons
A print on a glass bed.Photo: ENERGY.GOV ·Public domain ·Wikimedia Commons
ABS, bed 100 °C, open air: ABS · bed 100 °C · open air · corner lift 0.80 mm · warping.
ABS with a brim: ABS · bed 100 °C · open air · brim · corner lift 0.35 mm · warping.
ABS with a brim: ABS · bed 100 °C · open air · brim · corner lift 0.35 mm · warping.
Step 5: Control part cooling
The part cooling fan helps overhangs and small details, but on the first layers it cools the bottom too fast and pulls the corners up.
- Turn the fan off for the first 1–3 layers. Most PLA profiles already do this.
- For PETG, use less fan than for PLA.
- For ABS and ASA, use little or no fan, except for small details and bridges.
The hotend fan cools the heatsink. It must run whenever the hotend is hot.
A small fan cooling the extruder assembly.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
The print head: extruder on top, finned heatsink, heater block and nozzle.
Step 6: Stop drafts and keep the print warm
Moving air cools one side of the part faster than the other, and that uneven shrinking is what pulls corners up. Air conditioning, ceiling fans, open windows and even people walking past can be enough.
- Move the printer away from fans, air conditioning vents and windows.
- Use an enclosure for ABS, ASA and nylon. It keeps the air around the print warm and still. A cardboard box or a printer cover works for testing.
- Don’t open the enclosure door until the print is finished and the bed has cooled a little.
An enclosure keeps heat in for ABS and ASA.Photo: -stk ·CC BY-SA 4.0 ·Wikimedia Commons
An enclosed CoreXY printer on a home desk.Photo: Mortymore ·CC BY 2.0 ·Wikimedia Commons
A boxed dual-extrusion printer.Photo: Creative Tools from Halmstad, Sweden ·CC BY 2.0 ·Wikimedia Commons
An Ultimaker 3, a boxed desktop printer.Photo: DirkvdM ·CC BY-SA 4.0 ·Wikimedia Commons
A draft cools the part from one side.
ABS in a draft: ABS · bed 100 °C · fan draft · corner lift 1.17 mm · warping.
ABS in a draft: ABS · bed 100 °C · fan draft · corner lift 1.17 mm · warping.
Enclosed with a brim, the gauge reads no lift: ABS · bed 100 °C · enclosed · brim · corner lift 0.00 mm · flat.
ABS in an enclosure: ABS · bed 100 °C · enclosed · corner lift 0.28 mm · slight lift.
ABS in an enclosure: ABS · bed 100 °C · enclosed · corner lift 0.28 mm · slight lift.
ABS enclosed, with a brim: ABS · bed 100 °C · enclosed · brim · corner lift 0.00 mm · flat.
ABS enclosed, with a brim: ABS · bed 100 °C · enclosed · brim · corner lift 0.00 mm · flat.
Step 7: Choose a material that warps less
If a part keeps warping and it doesn’t need heat resistance, print it in a lower-shrink material.
| Material | Warp tendency | Bed temperature (typical) | Enclosure | Notes |
|---|---|---|---|---|
| PLA | Low | 55–65 °C | Not needed | Easiest for big, flat parts |
| PETG | Low–medium | 70–85 °C | Not needed | Grips PEI very hard; use glue stick or a release layer on smooth PEI |
| TPU | Low | 40–60 °C | Not needed | Flexible, rarely warps |
| ABS | High | 95–110 °C | Recommended | Needs warm, still air |
| ASA | High | 95–110 °C | Recommended | Like ABS, better outdoors |
| Nylon | Very high | Varies | Needed | Also needs very dry filament |
PLA: the beginner's filament.Photo: Richardspa ·CC0 ·Wikimedia Commons
Flexible filament: label shows its print temperature.Photo: Sweetclara ·CC BY-SA 4.0 ·Wikimedia Commons
A spool of ABS.Photo: Tatár Lehel ·CC BY-SA 3.0 ·Wikimedia Commons
Filament comes in almost every colour.Photo: westonhighschool library ·CC BY-SA 2.0 ·Wikimedia Commons
PLA, bed 60 °C: PLA · bed 60 °C · open air · corner lift 0.00 mm · flat.
PLA on a cold bed: PLA · bed 20 °C · open air · corner lift 0.62 mm · warping.
ABS, bed 100 °C, open air: ABS · bed 100 °C · open air · corner lift 0.80 mm · warping.
Step 8: Design and orient parts to resist warping
Shape matters. Long, wide, flat parts with sharp corners warp the most, because the shrinking pull is biggest along long edges and concentrates at sharp corners.
- Round sharp corners on the bottom edge (a few millimetres of fillet helps).
- Rotate the part so a smaller face sits on the bed, if it still prints well that way.
- Split very large parts into pieces that are glued or bolted together.
- Add thin “mouse ear” discs to the model’s corners if your slicer has no ears option.
A printed maze puzzle.Photo: Sumanbargavr ·CC BY-SA 4.0 ·Wikimedia Commons
A working wrench printed in one piece.Photo: Creative Tools from Halmdstad, Sweden ·CC BY 2.0 ·Wikimedia Commons
A screw-top box: threads print well at 0.2 mm layers.Photo: syvwlch ·CC BY 2.0 ·Wikimedia Commons
A printed bowl: walls only, no infill.Photo: Sumanbargavr ·CC BY-SA 4.0 ·Wikimedia Commons
A twisted vase printed in a single wall.Photo: Sumanbargavr ·CC BY-SA 4.0 ·Wikimedia Commons
Inside a print: 40% grid infill.Photo: Sumanbargavr ·CC BY-SA 4.0 ·Wikimedia Commons
Where to find these settings in your slicer
| Setting | OrcaSlicer / Bambu Studio | PrusaSlicer | Cura |
|---|---|---|---|
| Brim | Process → Others → Brim type and width | Print Settings → Skirt and brim → Brim width | Build Plate Adhesion → Adhesion Type: Brim |
| Raft | Process → Support → Raft layers | Print Settings → Support material → Raft layers | Build Plate Adhesion → Adhesion Type: Raft |
| Fan on first layers | Filament settings → Cooling → No cooling for the first layers | Filament Settings → Cooling → Disable fan for the first layers | Cooling → Initial Fan Speed |
| Bed temperature | Filament settings → bed temperature (per plate type) | Filament Settings → Filament → Bed | Material → Build Plate Temperature |
| First layer speed | Process → Speed → First layer | Print Settings → Speed → First layer speed | Speed → Initial Layer Speed |
Menu names move between slicer versions. If you can’t find a setting, type its name into the slicer’s settings search box.
When warping won’t go away
If you’ve worked through every step and corners still lift:
- Check the bed is flat. A warped bed or a bent build plate leaves gaps a brim can’t fix.
- Check the bed is heating evenly. Many beds are cooler at the edges than in the middle; raise the temperature a little or print nearer the centre.
- Try a different surface. Textured PEI, smooth PEI and glass grip different materials differently.
- Dry the filament. Wet filament prints weaker layers that can split.
- Change material. Some parts are simply too big and flat to print in ABS without a heated enclosure.
Your action plan
- Clean the plate before every print.
- Check the first layer and level the bed.
- Use the right bed temperature.
- Add a brim (or mouse ears) to big, flat or sharp-cornered parts.
- Keep the fan off for the first layers.
- Block drafts; enclose ABS and ASA.
- Round corners and choose a lower-shrink material when you can.
FAQ
Why do only the corners of my print lift?
Corners are where the shrinking pull comes from two directions at once, so they’re the first place to let go of the bed. Rounding the corners, adding a brim or mouse ears, and keeping the print warm all reduce that pull.
Does a hotter bed always stop warping?
No. A warmer bed helps the bottom layers stay stuck, but past the recommended range PLA softens and squashes at the bottom, and it doesn’t stop drafts cooling the top. Use the filament maker’s range and fix cleaning and drafts first.
Is glue stick a good idea?
On glass, often yes: it helps PETG and ABS grip and also stops PETG bonding too hard. On PEI it’s usually not needed for PLA, but a thin layer is a common release layer for PETG on smooth PEI.
Do I need an enclosure to stop warping?
Not for PLA, PETG or TPU in a draft-free room. For ABS, ASA and nylon an enclosure is the most reliable fix, because it keeps the air around the print warm and still.
Why does my print warp halfway through?
Usually a draft, or the part cooling fan ramping up after the first layers. Long prints are also more likely to meet a change in room temperature, like an air conditioner turning on.
Is warping the same as the first layer not sticking?
No. Warping lifts the edges of a part whose first layer did stick; a first layer that never sticks is an adhesion problem. They share fixes (clean bed, right Z offset), so start with first layer not sticking if the part comes loose early.
Can I flatten a warped print?
Sometimes, gently, with a heat gun and a flat weight, but the result is rarely as good as a re-print. It’s usually quicker to fix the cause and print again.
Related guides
- First layer not sticking? How to fix bed adhesion
- What is Z offset and how to set it
- How to level a 3D printer bed